Electrical discharge machining of titanium alloy (Ti–6Al–4V)

Electrical discharge machining of titanium alloy (Ti–6Al–4V). 任課教師 : 戴子堯 報告人:蔡雅雯 報告日期: 100.05.23. 大綱. 一、前言 二、實驗方法 三、結果與討論 四、結論. 一、前言. 一、前言. 放電加工是將工件及電極置於絕緣液中,通以適當電流,當電極與工件表面凹凸不平之高點接近至某一間隙時,其電壓增高,而電場強度引起該不平點之絕緣油的局部電離分解,因而產生火花放電,經由放電火花之高熱可將工件材料熔融或汽化而除去

rasha
Download Presentation

Electrical discharge machining of titanium alloy (Ti–6Al–4V)

An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. Electrical discharge machining of titanium alloy (Ti–6Al–4V) 任課教師:戴子堯 報告人:蔡雅雯 報告日期:100.05.23

  2. 大綱 一、前言 二、實驗方法 三、結果與討論 四、結論

  3. 一、前言

  4. 一、前言 • 放電加工是將工件及電極置於絕緣液中,通以適當電流,當電極與工件表面凹凸不平之高點接近至某一間隙時,其電壓增高,而電場強度引起該不平點之絕緣油的局部電離分解,因而產生火花放電,經由放電火花之高熱可將工件材料熔融或汽化而除去 • 本研究主要是探討以Ti-6Al-4V為放電加工之工件,在經過不同的加工參數和不同電極材料後之性質 • 實驗結果以SEM、EDS、XRD等來分析

  5. 二、實驗方法

  6. 二、實驗方法 • 實驗材料-Ti-6Al-4V(4.7 mm x 20 mmx 25mm) • 機械性質-Ti-6Al-4V

  7. 二、實驗方法 • 電極材料性質 electrode holder electrode • EDM之加工參數 specimen sample holder. EDM configuration

  8. 三、結果與討論

  9. 三、結果與討論 • 表面形貌分析 EDS analysis of machined surface, on which the EDS is conducted marked by A A typical surface after EDM (IP: 12 A; τON: 100 μs; electrode material copper). X-ray diffraction profiles of Ti–6Al–4V before machining

  10. 三、結果與討論 • XRD分析 • 煤油加工液分解成C和HC滲進工件表面TiC碳化物 X-ray diffraction profiles of Ti–6Al–4Vafter machining EDM (IP: 25 A; τON: 200 μs; electrode material copper).

  11. 三、結果與討論 • 白層截面微結構分析 • 白層厚度約10-20μm,結構為麻田散鐵組織 Cross-sectional view of white EDM (IP: 6 A; τON: 100 μs; electrode material graphite).

  12. 三、結果與討論 • 平均白層厚度(whitelayer thickness, WLT)分析 • 隨著放電持續時間的恆定電流增加,可看出白層的平均厚度有明顯增加的趨勢 Effect of EDM parameters on average WLT (a) graphite electrode; (b) copper electrode; (c) aluminium electrode.

  13. 三、結果與討論 • 表面裂紋分析 • 脈衝電流↑放電持續時間↓ 表面裂紋↓ Effect of EDM parameters on surface crack density ((★) extremely open cracks; (◇) slightly cracks; (○) no crack).

  14. 三、結果與討論 • 表面粗糙度分析 • 鋁>銅>石墨 • 電流↑表面粗糙度↑ • 隨著放電持續時間增加(200μs)表面粗糙度有略為改善的現象 Effect of EDM parameters on surface roughness of specimens ((a) graphite electrode; (b) copper electrode; (c) aluminium electrode).

  15. 三、結果與討論 • 電極損耗率分析 • 脈衝電流↑ 、放電持續時間↑ 電極損耗率↑ 石墨電極損耗率較低

  16. 三、結果與討論 • 材料移除率分析 • 脈衝電流↑ 、放電持續時間↑ 材料移除率↑ • 石墨電極材料移除率較佳 Effect of EDM parameters on MRR ((a) graphite electrode; (b) copper electrode; (c) aluminium electrode).

  17. 四、結論

  18. 四、結論 • 由於Ti-6Al-4V的熱傳導係數較低,使得放電加工過程中,會形成再鑄層(白層),因含有TiC碳化物,其硬度相當高 • 隨著放電加工參數的增加,平均白層厚度也隨之增加,也隨著電極材料的不同而有所影響,實驗結果發現以銅為電極材料來做加工,工件表面產生裂紋的機率較高 • 石墨電極因具有高熔點,以至於放電加工時,其電極損耗率較低,材料移除率較高