M. Kopcewicz and T. Kulik a )

Rf-Mössbauer study of the magnetic properties of nanocrystalline FeNiZrB and FeNiCoZrB alloys. M. Kopcewicz and T. Kulik a ). Institute of Electronic Materials Technology, 01-919 Warszawa, Wólczyńska Street 133, Poland,

pilar
Download Presentation

M. Kopcewicz and T. Kulik a )

An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. Rf-Mössbauer study of the magnetic properties of nanocrystalline FeNiZrB and FeNiCoZrB alloys M. Kopcewicz and T. Kulik a) Institute of Electronic Materials Technology, 01-919 Warszawa, Wólczyńska Street 133, Poland, a) Faculty of Materials Science and Engineering, Warsaw University of Technology, 02-507 Warszawa, Wołoska Street 141, Poland,

  2. Introduction Nanocrystalline alloys are excellent soft magnetic materials with wide practical applications [1]. The main disadvantage: high brittleness. FeNiZrB alloy: show improved mechanical properties but at the expense of saturation magnetization of nanograins [2]. In order to increase the magnetization - Co is added. Aim of the current study: Investigation of magnetic properties of the nanocrystalline alloys: Fe31Ni50Zr7B12 (Co-free alloy) and Fe41Ni40-xCoxZr7B12 (x=10, 20) (Co10 and Co20 alloys) by means of the rf-Mössbauer technique. This technique permits us to study changes of magnetic anisotropy and to follow the variations of magnetostriction associated with the formation of nanocrystalline grains.

  3. Experimental procedure Samples:amorphous alloysFe31Ni50Zr7B12 (Co-free alloy), Fe41Ni30Co10Zr7B12 (Co10 alloy), and Fe41Ni20Co20Zr7B12 (Co20 alloy), prepared by the melt quenching technique. The ribbons: 3 to 5 mm wide and about 25 m thick. The nanocrystalline alloys: formed by 1 hour annealing in vacuum of amorphous precursors (annealing temperatures: Ta= 440 –770oC). The rf-Mössbauer measurements: performed during sample exposure to a radio frequency (rf) magnetic field with a frequency of 61 MHz, and the intensity of which was varied between 0 and 20 Oe. The rf field was applied in the plane of the sample. The rf-Mössbauer investigations were accompanied by measurements of quasi-static hysteresis loops.

  4. Rf-Mössbauer technique combines the Mössbauer effect with phenomena induced by an external radio-frequency magnetic field in ferromagnetic materials (see e.g., [3, 4, 5]). Effects induced by the rf field: 1. RF-SIDEBANDS EFFECT 2. RF-COLLAPSE EFFECT

  5. Rf-Mössbauer technique 1. RF-SIDEBANDS EFFECT - frequency modulation of Mössbauer -radiation due to rf-induced vibrations of Mössbauer atoms via magneto-acoustic coupling - magnetostriction Sidebands positions - given by nr intensities - frequency modulation (FM) model Rf-sidebands can be observed in ferromagnetic magnetostrictive materials (below the Curie point)

  6. 2. RF-COLLAPSE EFFECT - magnetic radio-frequency field Hrf larger than the anisotropy field HA (Hrf > HA) - rf frequency rf larger than Larmor frequency L(rf > L)  fast reversal of magnetization  fast relaxation of the hyperfine field  hyperfine field is averaged to zero Magnetic hyperfine structure in Mössbauer spectrum disappears  the rf-collapsed spectrum: only QS doublet or a single line (the sample is in the ferromagnetic state). RF-collapse - very sensitive to the relation between Hrf and HA - thus HA can be scanned by changing Hrf RF-collapse can be observed in soft ferromagnetic materials Rf-collapse allows the separation of magnetic dipole and electric quadrupole hyperfine interactions in the ferromagnetic state

  7. Rf-Mössbauer Results 1. Co-free alloy Conventional Mössbauer spectra : - as-quenched alloy- fully amorphous - nanocrystallization: at 470 – 670oC The dominating phase - bcc-FeNi accompanied by the (FeNi)23B6 phase. Rf-Mössbauer spectra - the as-quenched alloy and annealed at Ta= 470oC - rf-spectra - a collapsed doublet accompanied by rf sidebands. The alloy is magnetically very soft and magnetostrictive. - at Ta 520oCthe collapsed pattern - single line - very soft bcc-FeNi phase; the rf sidebands vanished. - at Ta 570oC - rf-collapse incomplete. The Mössbauer spectra recorded before and after rf exposure are identical.

  8. 2. Co-containing alloys Co10 alloy: As-quenched alloy: Addition of Co to the amorphous structureincreases the anisotropy field. -The full collapse of mhfs occurs at higher intensity of the rf field (16 Oe). -The rf-sidebands of high intensity are observed. -A larger Co-content causes the instability of the amorphous phase during exposure to the rf field as a result of which the amorphous alloy crystallizes partly due to the rf field exposure. Co-containing nanocrystalline alloys: The anisotropy field strongly increased. -The rf-spectra of Co10 alloy (Ta470-570oC, rf field 20 Oe at 61 MHz) - a central doublet accompanied by partially narrowed mhfs. - No rf-sidebands. - At Ta=620oC: rf-spectra do not depend on the rf field intensity and show mhfs of FeCo phase (no rf-collapse, no rf-sidebands).

  9. Co20 alloy: As-quenched alloy: - rf collapsed pattern +intense rf sidebands Annealed alloy: - at Ta 520oC: noncollapsed mhfs (FeCo phase) (large anisotropy limits the rf collapse) + collapsed doublet (amorphous matrix) - at Ta = 620oC: rf-spectra do not depend on the rf field - mhfs of FeCo phase large anisotropy field The magnetostriction of the nanocrystalline alloy vanished; the rf sidebands are not observed.

  10. The Mössbauer spectra recorded (without rf field) for the alloys (Co-free and Co-containing) before and after the rf field exposure: - are identical in the case of Co-free alloys, i.e., no rf induced crystallization; - are significantly different in the case of Co-containing alloys - rf- induced crystallization. The rf induced crystallization is attributed to mechanical deformations induced in the sample via magnetostriction (rf-sidebands effect).

  11. Measurements of the quasi-static hysteresis loops [6] - the magnetic induction B (magnetization) and coercive fields HC were estimated. The coercivity in the Co-containing alloys strongly increased after annealing: Co20-alloy: The smallest coercivity, 15 A/m was observed at Ta=520oC, then increased to 783 A/m (Ta=570oC) and 4726 A/m (Ta=620oC). The largest value (13113 A/m) was reached at Ta=670oC. The changes in coercivity reflect the FeCo phase abundance in the alloys. The hysteresis loops recorded for Fe41Ni20Co20Zr7B12 alloy The measurements of the hysteresis loops fully support the rf-Mössbauer results.

  12. Conclusions • The rf-Mössbauer results show that: • The amorphous precursors are magnetically very soft. • The anisotropy field increases with the introduction of Co • - in the amorphous alloy - this effect is significant • - in nanocrystalline alloys - this increase is dramatic. • The rf-Mössbauer measurements are very useful for the estimation of magnetic anisotropy fields. • The presence and the magnitude of the rf sidebands provide direct information regarding the magnetostriction of the alloys. • The rf sidebands vanish when the magnetostriction becomes negligible due to formation of the nanocrystalline structure. • A novel effect - the rf-induced crystallization, of nonthermal origin, of Co-containing alloys attributed to magnetostriction.

  13. The rf field applied was able to induce the fast magnetization reversal (rf-collapse) only if the rf field intensity was markedly larger than the anisotropy field. The rf-collapse effect was suppressed when the anisotropy field became comparable to or larger than the rf field intensity. In the Co-containing alloys both coercive fields and anisotropy fields strongly increase at higher annealing temperatures.

  14. References: 1. A. Makino, T. Hanai, A. Inoue, T. Masumoto, Mater. Sci. Eng. A 179/180, 552 (1994). 2. M. Kopcewicz, B. Idzikowski, J. Kalinowska, J. Appl. Phys. 94, 638 (2003). 3. M. Kopcewicz, Strutural Chem. 2, 313 (1991). 4. M. Kopcewicz, in G.J. Long, F. Grandjean (Eds) "Mössbauer Spectroscopy Applied to Inorganic Chemistry" vol. 3, Plenum, N. York, London, 1989, p. 243. 5. M. Kopcewicz, J. Alloys and Comp. 382, 165 (2004). 6. T. Kulik, H.T. Savage, A. Hernando, J. Appl. Phys. 73, 6855 (1993). These results were presented at the Magnetism and Magnetic Materials Conference (MMM-2005), San Jose, CA, (USA) in November 2005 and were published in the Journal of Applied Physics 99, 08F112 (2006).